Key facts
- Pickled and oiled hot rolled coil: EN 10111, EN 10025-2 and EN 10149-2. Cold rolled coil: EN 10130.
- Galvanized and Aluzinc coil: EN 10346 (coating codes Z and AZ) or, in ASTM, A653/A653M and A792/A792M.
- Prepainted coil: EN 10169 for the paint coating, with the metal substrate following EN 10346.
- EN 10111 covers 1.0 to 11 mm (0.039 to 0.433 in) [0.039 to 0.43 in]. EN 10130 covers 0.35 to 3 mm (0.014 to 0.12 in) [0.014 to 0.118 in] in widths of 600 mm (23.62 in) [23.6 in] and over. EN 10346 covers 0.20 mm to 6.5 mm (0.008 to 0.256 in) [0.008 to 0.256 in] in the scope published by BSI, and thinner strip by agreement. Check the current edition of each standard before you rely on a range.
- In an enquiry the standard, the grade, the coating designation and the dimensions are stated together.
Which standard applies to which coil product?
A standard in this field is a set of technical delivery conditions: it defines what product it covers, which grades exist, and what the buyer states when ordering. Every coil product sold here has one main standard, and the coated ones have two layers. The table below shows the match; the product pages give the sourcing ranges.
| Product | Standards | Grades on the product page |
|---|---|---|
| Pickled and oiled hot rolled coil | EN 10111, EN 10025-2, EN 10149-2 | DD11 to DD14; S235JR, S275JR, S355JR; S315MC to S700MC |
| Cold rolled coil | EN 10130 | DC01, DC03, DC04, DC05, DC06 |
| Galvanized coil | EN 10346 (Z); ASTM A653/A653M | DX51D+Z to DX57D+Z; S220GD+Z to S550GD+Z |
| Aluzinc coil | EN 10346 (AZ); ASTM A792 | Coating AZ100 to AZ185; base grade confirmed with the mill |
| Prepainted coil | EN 10169 and the substrate standard EN 10346 | DX51D+Z to DX54D+Z; S220GD+Z to S350GD+Z |
The same chain is visible in the standards themselves. EN 10130 is about uncoated cold rolled steel, and its scope leaves coated products to other standards. EN 10346 notes that its coated products can be used as substrates for the organic coated products of EN 10169, and EN 10169 lists EN 10111, EN 10130 and EN 10346 among its references. For how hot rolled and cold rolled coil differ as products, read hot rolled vs cold rolled coil.
What do EN 10111, EN 10025-2 and EN 10149-2 cover?
These are the three hot rolled standards on the pickled and oiled hot rolled coil page, and they answer three different needs.
- EN 10111 specifies continuously hot rolled low carbon steel sheet and strip in coils for cold forming, for each grade with chemical composition and mechanical properties. It applies to thicknesses of 1.0 mm to 11 mm (0.039 to 0.433 in) [0.039 to 0.43 in]. The forming grades sold under it are written DD11 to DD14 on the product page. It excludes products covered by other standards, including the structural steels of EN 10025.
- EN 10025-2 specifies technical delivery conditions for hot rolled flat and long products of non-alloy quality structural steels. Structural grades such as S235JR, S275JR and S355JR are listed on the product page under this standard. S marks structural steel, and the number is the minimum yield strength in MPa as EN 10027 names steels; the letters after the number (such as JR) refer to impact properties.
- EN 10149-2 specifies weldable, hot rolled, high yield strength steels for cold forming in the thermomechanically rolled condition. Its scope gives 1.5 to 20 mm (0.059 to 0.787 in) [0.059 to 0.79 in] for yield strengths of 315 to 460 MPa and 1.5 to 16 mm (0.059 to 0.630 in) [0.059 to 0.63 in] for 500 to 700 MPa. The product page lists S315MC to S700MC.
The pickled and oiled range sourced here starts at 0.80 mm (0.031 in) [0.031 in], below the 1.0 mm (0.039 in) lower limit of EN 10111. That is why thickness is stated together with the standard in an enquiry, and the mill confirms the combination.
What does EN 10130 cover for cold rolled coil?
EN 10130 applies to cold rolled uncoated low carbon steel flat products for cold forming, delivered as sheet, coil, slit coil or cut lengths. It applies to rolled widths of 600 mm (23.62 in) [23.6 in] and over, in a thickness of 0.35 mm (0.014 in) [0.014 in] up to 3 mm (0.12 in) [0.118 in] unless otherwise agreed at enquiry and order. It does not apply to cold rolled narrow strip below 600 mm (23.62 in), and it leaves out products with their own standards, among them high yield strength cold forming products (EN 10268), vitreous enamelling products (EN 10209) and magnetic steel.
The grades start with DC01 (the product page lists DC01, DC03, DC04, DC05 and DC06). The first letter D follows the EN 10027 pattern for flat products for cold forming. Tolerances are not in EN 10130: they are in the companion standard EN 10131. The thickness at which the standard starts (0.35 mm (0.014 in)) is above the lower end of the cold rolled range sourced here (0.20 mm (0.008 in) [0.008 in]), so state both the standard and the thickness.
What does EN 10346 cover for galvanized and Aluzinc coil?
EN 10346 is the European standard for continuously hot-dip coated steel flat products for cold forming. The scope published by BSI lists low carbon steels for cold forming, steels for construction and steels with high proof strength for cold forming, coated with zinc (Z), zinc-iron (ZF), zinc-aluminium (ZA), aluminium-zinc (AZ), zinc-magnesium (ZM), aluminium-silicon (AS) or aluminium (A), in thicknesses of 0.20 mm to 6.5 mm (0.008 to 0.256 in) [0.008 to 0.256 in]. By agreement at enquiry and order it also applies to strip thinner than 0.20 mm (0.008 in). It applies to strip of all widths and to sheets cut from it. The galvanized range sourced here (up to 4.00 mm (0.157 in) [0.157 in]) and the Aluzinc range both lie inside that scope, and the mill confirms the combination of grade, coating and thickness for each order. Scopes and grade tables are revised from time to time, so check the current edition.
How the designations read, from the standard text read for this guide and the product pages:
- DX51D to DX57D are the low carbon steels for cold forming, ranked by increasing suitability for forming: DX51D is bending and profiling quality, DX52D is drawing quality, DX53D is deep drawing quality, DX54D special deep drawing quality, DX56D extra deep drawing quality and DX57D super deep drawing quality. The suffix +Z (zinc) or +AZ (aluminium-zinc) names the coating. Check the current edition for the grade table.
- S220GD+Z to S550GD+Z are structural steels, ranked by increasing minimum proof strength. As EN 10027 names structural steels, the number is the minimum yield strength in MPa, and +Z is the coating. The range S220GD to S550GD is the one listed on the product page, so confirm the grade with the mill.
- The coating mass is the nominal total for both surfaces in g/m². Combined with the coating code it is the coating designation, so Z275 is 275 g/m² and AZ150 is 150 g/m². The details are in galvanized vs Aluzinc coil, and the names Galvalume, Zincalume and Aluzinc are explained in Galvalume, Zincalume and Aluzinc coil.
ASTM has two matching standards. A653/A653M covers steel sheet, zinc-coated (galvanized) or zinc-iron alloy-coated (galvannealed) by the hot-dip process in coils and cut lengths, and A792/A792M covers 55% aluminum-zinc alloy-coated steel sheet in coils and cut lengths. A792 states that its product is intended for applications requiring corrosion resistance, heat resistance, or both. In ASTM the coating is given as a designation in oz/ft², and one oz/ft² equals 305 g/m² in ASTM usage, so US and metric orders can be matched on coating mass, but the grade systems differ.
What does EN 10169 cover for prepainted coil?
EN 10169 specifies requirements for continuously organic coated (coil coated) steel flat products, and in particular the performance requirements of the coating. It covers wide strip, sheet cut from wide strip, slit wide strip, strip rolled in widths below 600 mm (23.62 in) and cut lengths. It is not applicable to tin mill products or electrical steels.
The standard does not make the steel. The substrate is a metal product from another standard: the references of EN 10169 include EN 10111, EN 10130, EN 10152 (electrolytically zinc coated) and EN 10346, and for prepainted steel coil the base is galvanized strip to EN 10346. A prepainted order therefore names two things: the substrate grade and coating, and the paint requirements. The colour, gloss and paint system are specified separately as the product page describes, and the paint families are covered in prepainted coil paints and RAL colours.
The standard measures the coating with the EN 13523 series of coil coated metals test methods, such as film thickness, gloss, colour difference, bending, adhesion, salt spray and UV resistance. Its newest edition added a requirement of a maximum of six months between production and processing of the coil coated product, so ask about the age of the coil if you will store it.
How do EN and ASTM standards relate?
They cover the same families of products, but they are separate systems. The coating types correspond (Z and AZ in EN 10346, zinc-coated and 55% aluminum-zinc in ASTM A653 and A792), and the coating can be compared through its mass per area. They differ in how grades are named, in tests and in dimensional tolerances, so this guide makes no claim that a given EN grade equals a given ASTM grade. For the US reader, write the ASTM designation you need, for example the coating designation in oz/ft², and the mill answers whether it can supply it, or offers the nearest EN grade for you to approve.
What should you state in a coil enquiry?
The EN 10346 text read for this guide lists what a purchaser states at enquiry and order, among them the quantity, the type of product, the dimensional standard (EN 10143), the nominal dimensions, the number of the standard, the steel name with the coating symbol, the coating mass, the coating finish, the surface quality and the surface treatment (for example oiled). For coil, a working list is:
- Product (pickled hot rolled, cold rolled, galvanized, Aluzinc, prepainted).
- Standard and grade, with the coating suffix and coating mass for coated coil.
- Thickness and width in millimetres, full-width coil or slit coil.
- Coil inner diameter, maximum coil weight, quantity and destination. The steel coil weight calculator turns weight, width and thickness into length and outer diameter.
- For prepainted coil: the paint system, colour, gloss, and top and reverse side.
- The end use, because it decides the grade and the coating.
For packing, labelling and container loading, read steel coil packing and container loading. Send the enquiry through the quote request. Reinwent is a trading and sourcing company, and this coil is sourced from manufacturers in Türkiye. The quotation follows within 12 hours at the latest. The whole range is on the steel coil page.
Read next: steel coil FAQ, steel coil: Türkiye vs China, pickled and oiled steel, steel coil grades DX51D, DD11 and DC01, coil thickness and width selection, cold rolled coil annealing and surface quality, steel coil HS codes, steel coil importers guide.

Steel